Grade 32Cr3Mo
China ISC A30321
Corresponding Standard GB /T 37618-2019
Nitriding steels
Classification Alloy Steel
32Cr3Mo Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value 0.28 0.17 0.4 - - 2.8 - - 0.3
Maximum Value 0.35 0.37 0.7 0.03 0.03 3.3 0.3 0.3 0.5
32Cr3Mo Mechanical Properties
test size
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d=25 Quenching temperature 870~930°C, oil/water cooling; tempering temperature 580~700°C, water/oil cooling ≥1030 ≥835 ≥10 Normalizing + Tempering, Annealing or High Temperature Tempering Condition Delivered Steel Rod
≤248
≥25

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!