Grade 27ХГСНМДТЛ
Other Names
Corresponding Standard GOST 21357-1987
Castings Made of Cold-and Wear-Resistant Steel
Classification Cast Steel
27ХГСНМДТЛ Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo Ti
Minimum Value 0.22 0.7 0.9 - - 0.7 0.7 0.3 0.1 0.03
Maximum Value 0.31 1.3 1.5 0.02 0.02 1.3 1.2 0.5 0.3 0.07
27ХГСНМДТЛ Mechanical Properties
form Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Casting Normalizing 910~930°C, Tempering 590~610°C ≥800 ≥650 ≥12 ≥20 KCV-60: ≥3KJ/m2
KCU-60: ≥5KJ/m2
Casting Quenching 910~930°C, water cooling, Tempering 640~660°C ≥850 ≥700 ≥12 ≥25 KCV-60: ≥3.5KJ/m2
KCU-60: ≥5KJ/m2
Casting Quenching 910~930°C, water cooling, Tempering 200~220°C ≥1400 ≥1150 ≥8 ≥12 ≥390 KCV-60: ≥2.5KJ/m2
KCU-60: ≥4KJ/m2

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!