Grade 09CuPCrNi-B
Corresponding Standard TB /T 1979-2003
Technical specification for the procurement of atmospheric corrosion resisting steel for railway rolling stock
Classification Alloy Steel
09CuPCrNi-B Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu
Minimum Value - 0.1 0.2 0.06 - 0.3 0.25 0.25
Maximum Value 0.12 0.4 0.5 0.12 0.02 0.65 0.5 0.45
09CuPCrNi-B Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤6 Hot Rolling ≥431 ≥295 ≥24
t>6 Hot Rolling ≥431 ≥295 ≥24 t ≥ 12:
Room Temperature: ≥47
-40°C: ≥21
t≤4 Cold Rolling ≥402 ≥265 ≥27
09CuPCrNi-B Corresponding Standards(Same grade name, different standards)