Grade EN-GJS-350-22
European Standard Steel Grade 5.3102
Other Names
Corresponding Standard EN 1563-2018
Classification cast Iron
Density 7.1 g/cm3
EN-GJS-350-22 Mechanical Properties
condition Mark
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Casting specimen; t≤30 EN-GJS-350-22 ≥350 ≥220 ≥22
Casting specimen; 30<t≤60 EN-GJS-350-22 ≥330 ≥220 ≥18
Casting samples; 60<t≤200 EN-GJS-350-22 ≥320 ≥210 ≥15
Base specimen; t≤30 EN-GJS-350-22C ≥340 ≥220 ≥20
Base specimen; 30<t≤60 EN-GJS-350-22C ≥320 ≥210 ≥15
Test specimen; EN-GJS-350-22C ≥310 ≥200 ≥12
Castings; t≤60 <160
Castings; 60 < t ≤ 200 <160
• Samples cut from the casting the letter “C” is added at the end of the designation by symbol. e.g. EN-GJS-800-2C
Approximate Comparison Table Cast Iron
Japan International Organization for Standardization European Standard United Kingdom
JIS ISO EN Numerical Grade BS EN/BS
FCD350-22 350-22
350-22/S
350-22/U
EN-GJS-350-22 5.3102
(EN-JS1010)
350/22

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!