Grade GS-33NiCrMo 7 4 4
Germany W-Nr. 1.6740
Corresponding Standard DIN 17205-1992
Quenched and Tempered Steel Castings for General Applications Technical Delivery Conditions
Classification Cast Steel
GS-33NiCrMo 7 4 4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.3 - 0.5 - - 0.9 1.5 0.35
Maximum Value 0.36 0.6 0.8 0.015 0.007 1.2 1.8 0.5
GS-33NiCrMo 7 4 4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤150 Vacuum Quenching + Tempering 800~950 ≥600 ≥12 ≥32
150<t≤400 Vacuum Quenching + Tempering 750~900 ≥550 ≥12 ≥32