Grade G26CrMo4
Germany W-Nr. 1.7221
Corresponding Standard DIN EN 10293-2005
Steel castings for general engineering uses
Classification Cast Steel
G26CrMo4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo
Minimum Value 0.22 - 0.5 - - 0.8 0.15
Maximum Value 0.29 0.6 0.8 0.025 0.02 1.2 0.3
• For castings of ruling thickness < 28 mm, S ≤ 0,030 % (by mass) is permitted.
G26CrMo4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤100 Quenching + tempering (+QT1)
Quenching temperature 880~950°C, air or water cooling, tempering temperature 600~650°C
600~750 ≥450 ≥16 ≥40
100<t≤250 Quenching + tempering (+QT1)
Quenching temperature 880~950°C, air or water cooling, tempering temperature 600~650°C
550~700 ≥300 ≥14 ≥27
t≤100 Quenching + Tempering (+QT2)
Quenching temperature 880~950°C air or liquid cooling, Tempering temperature 550~600°C
700~850 ≥550 ≥10 ≥18
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17205-1992
Grade
Germany W-Nr.
DIN EN 10293-2005
Grade
Germany W-Nr.
G26CrMo4 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!