Grade G30CrMoV6-4
Germany W-Nr. 1.7725
Corresponding Standard DIN EN 10293-2005
Steel castings for general engineering uses
Classification Cast Steel
G30CrMoV6-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo V
Minimum Value 0.27 - 0.6 - - 1.3 0.3 0.05
Maximum Value 0.34 0.6 1 0.025 0.02 1.7 0.5 0.15
G30CrMoV6-4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤100 Quenching + tempering (+QT1)
Quenching temperature 880~950°C, water cooling, tempering temperature 600~650°C
850~1000 ≥700 ≥14 ≥45
100<t≤150 Quenching + tempering (+QT1)
Quenching temperature 880~950°C, water cooling, tempering temperature 600~650°C
750~900 ≥550 ≥12 ≥27
150<t≤250 Quenching + tempering (+QT1)
Quenching temperature 880~950°C, oil cooling, tempering temperature 600~650°C
650~800 ≥350 ≥12 ≥20
t≤100 Quenching + Tempering (+QT2)
Quenching temperature 880~950°C liquid cooling, Tempering temperature 530~600°C
900~1100 ≥750 ≥12 ≥31
New and Old Grade Replacement List
Corresponding Standard Grade
DIN 17205-1992
Grade
Germany W-Nr.
DIN EN 10293-2005
Grade
Germany W-Nr.
G30CrMoV6-4 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!