Grade G20NiMoCr4
Germany W-Nr. 1.6750
Corresponding Standard DIN EN 10293-2005
Steel castings for general engineering uses
Classification Cast Steel
G20NiMoCr4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value 0.17 - 0.8 - - 0.3 40.8 0.4
Maximum Value 0.23 0.6 1.2 0.025 0.015 0.5 1.2 0.8
G20NiMoCr4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤150 Quenching + Tempering (+QT)
Quenching temperature 880~930°C air or liquid cooling, Tempering temperature 650~700°C
570~720 ≥410 ≥16 -45°C: ≥27
Room temperature: ≥40
G20NiMoCr4 Corresponding Standards(Same grade name, different standards)