Grade GX3CrNi13-4
Germany W-Nr. 1.6982
Corresponding Standard DIN EN 10293-2005
Steel Castings for General Engineering Uses
Classification Cast Steel
GX3CrNi13-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo
Minimum Value - - - - - 12 3.5 -
Maximum Value 0.05 1 1 0.035 0.015 13.5 5 0.7
GX3CrNi13-4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤300 Quenching + Tempering (+QT)
Quenching temperature 1000~1050°C air cooling, Tempering temperature 670~690°C air cooling + 590~620°C
700~900 ≥500 ≥15 -120°C: ≥27
GX3CrNi13-4 Corresponding Standards(Same grade name, different standards)