Grade 5086
Corresponding Standard ASME SB-928/SB-928M-2023
High Magnesium Aluminum-alloy sheet and plate for marine service and similar environments
Classification Aluminum and Aluminum Alloys
5086 Chemical Element Composition Content (%)
Component Fe Si Mn Cr Cu Ti Zn Mg Other Individual Other Total More
Minimum Value - - 0.2 0.05 - - - 3.5 - - Al:余量
Maximum Value 0.5 0.4 0.7 0.25 0.1 0.15 0.25 4.5 0.05 0.15
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
5086 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
1.6<t≤6.3 Strain - Only Hardening (H116) 275~360 ≥195 L0=50mm: ≥8
6.3<t≤12.5 Strain - Only Hardening (H116) 275~360 ≥195 L0=50mm: ≥10
12.5<t≤30 Strain - Only Hardening (H116) 275~360 ≥195 L0=5D: ≥9
30<t≤50 Strain - Only Hardening (H116) 275~360 ≥195 L0=5D: ≥9
1.6<t≤6.3 Strain - Hardening and Stabilization (H321) 275~355 ≥195 L0=50mm: ≥8
6.3<t≤8 Strain - Hardening and Stabilization (H321) 275~355 ≥195 L0=50mm: ≥9
Approximate Comparison Table Aluminium and Aluminium Alloy
Japan United States International Organization for Standardization Germany France European Standard Russia
JIS ASTM ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST
5086 5086 AlMg4Mn AlMg4Mn 3.3545 5086
A-G4MC
ENAW-AlMg4 ENAW-5086 AMg4
AMg4.5

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!