Grade En56BM
Corresponding Standard BS 970-1955
Wrought steels in the form of bars, billets and forgings up to 6 in. ruling section for automobile and general engineering purpose
Classification Martensitic Stainless Steel
En56BM Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo Zr Pb Se More
Minimum Value 0.12 - - - - 12 - - - - - Mo+Zr+Pb+Se≤1
Maximum Value 0.18 1 1.5 0.045 0.75 14 1 0.6 0.6 0.35 0.6
En56BM Mechanical Properties
diameter or width across flats
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Bar, square bloom, forging; d≤152.4 Quenching and Tempering P ≥540 ≥20 152~207 ≥34
Bar, square bloom, forging; d≤152.4 Quenching and Tempering R ≥695 ≥15 201~255 ≥27
Bars, square billets, forgings; d≤101.6 Quenching and Tempering S ≥772 ≥12 223~277 -
• d-diameter or width across flats/mm
• The unit conversion for strength is based on: 1tons/sq.in=15.44N/mm2
• The unit conversion for impact energy absorption is based on: 1ft.lb=1.3558J
En56BM Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!