Grade ZG16Cr9Mo1
Corresponding Standard GB /T 32255-2015
General Martensitic Stainless Steel and Alloy Steel Castings Suitable for High Temperature and High Pressureservice
Classification Cast Steel
ZG16Cr9Mo1 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value 0.12 - 0.35 - - 8 - - 0.9 -
Maximum Value 0.19 1 0.65 0.03 0.03 10 0.4 0.3 1.2 0.05
ZG16Cr9Mo1 Mechanical Properties
thickness
t
mm
Test Temperature Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
Castings; t≤150 Room Temperature 960~1020°C Normalizing + 680~740°C Tempering 620~795 ≥415 ≥18 ≥27
Casting Normalizing + Tempering ≥375
Casting ≥355
Casting ≥345
Casting ≥320
Casting ≥295
Casting ≥265
Approximate Comparison Table Heat-Resistant Cast Steels and Alloys
China United States United Kingdom
GB ASTM BS EN/BS
ZG16Cr9Mo1
GB/T 32255-2015
C12
ASTM A217-2012
GX15CrMo9-1
BS EN 10213-2007

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!