Grade C45E
European Standard Steel Grade 1.1191
Corresponding Standard EN 10305-1-2010
Steel tubes for precision applications - Technical delivery conditions - Part 1: Seamless cold drawn tubes
Classification Carbon Steel
C45E Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo More
Minimum Value 0.42 - 0.5 - - - - Cr+Mo+Ni≤0.63
Maximum Value 0.55 0.4 0.8 0.03 0.035 0.4 0.1
C45E Mechanical Properties
condition Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Seamless steel pipe C45E +C Cold Drawn Hardened (+C) ≥720 ≥4
Seamless steel pipe C45E +LC Cold Precision Finished (+LC) ≥670 ≥6
Seamless steel pipe C45E +A Annealing (+A) ≥510 ≥20
Seamless steel pipe C45E +N Normalizing (+N) ≥540 ≥340 ≥18
1 Approximate Comparison Table Non-Alloy Steel for Quenching and Tempering
China Japan International Organization for Standardization European Standard
GB JIS ISO EN Numerical Grade
45 S45C C45E C45E 1.1191
2 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB JIS ASTM ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
45H
45
S45C 1045 C45E4 Ck45 XC45
XC48H1
C45E 1.1191 45 1672 080M46
CFS8
3 Approximate Comparison Table High-Quality Carbon Structural Steel
China Japan United States International Organization for Standardization European Standard
GB ISC JIS ASTM/AISI ISO EN Numerical Grade
45Mn
(GB/T 699-2015)
U21452 SWRH47B
(JIS G3506:2004)
1046
(ASTM A29/A29M:2005)
C45E4
(ISO 683-18:1996)
C45E
(EN 1008-1:1991+A1:1996)
(EN 10084:1998)
1.1191

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!