Grade 34CrNi3MoV
Corresponding Standard GB /T 33084-2016
Heavy Alloy Structural Steel Forgings-Technical Specification
Classification Alloy Steel
34CrNi3MoV Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value 0.3 0.17 0.5 - - 1.2 3 - 0.25 0.1
Maximum Value 0.4 0.37 0.8 0.025 0.025 1.5 3.5 0.2 0.4 0.2
34CrNi3MoV Mechanical Properties
diameter or thickness
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
d≤100 Tempering ≥900 ≥785 ≥14 ≥40 269~321 ≥47
100<d≤300 Tempering ≥855 ≥735 ≥14 ≥38 248~311 ≥39
300<d≤500 Tempering ≥805 ≥685 ≥13 ≥33 235~293 ≥31
500<d≤800 Tempering ≥735 ≥590 ≥12 ≥30 212~262 ≥31
34CrNi3MoV Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!