Grade 20CrMnTi
Corresponding Standard GB /T 17107-1997
Structural Steel Grades And Mechanical Property For Forgings
Classification Alloy Steel
20CrMnTi Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Ti
Minimum Value 0.17 0.17 0.8 - - 1 - - 0.04
Maximum Value 0.23 0.37 1.1 0.035 0.035 1.3 0.3 0.3 0.1
• High-quality steel——P≤0.035;S≤0.035;Cu≤0.3;Cr≤0.3;Ni≤0.3
• Extra-quality steel (Suffix A)——P≤0.025;S≤0.025;Cu≤0.25;Cr≤0.3;Ni≤0.3
• Special High-Quality Steel (Suffix E)——P≤0.025;S≤0.015;Cu≤0.25;Cr≤0.3;Ni≤0.3
20CrMnTi Mechanical Properties
diameter or thickness
d
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Impact Energy Absorption
KV2
J
d≤100 Sample Direction: Longitudinal Tempering ≥615 ≥395 ≥17 ≥45 ≥47
• The forgings must be inspected for mechanical properties after performance heat treatment and before any surface treatment.
• After the samples are removed, no heat treatments that affect the mechanical properties or any processing that influences the test results shall be conducted.
• Mechanical property testing primarily evaluates the material\'s tensile strength, impact resistance, and hardness. When conducting tensile, impact, and hardness tests simultaneously, the hardness value is for reference only. Alternatively, one may choose to perform only one of the tensile, impact, or hardness tests.
1 Approximate Comparison Table Structural Alloy Steel
China Germany Russia
GB ISC DIN EN/DIN W-Nr. GOST
20CrMnTi
30CrMnTi
A26202
A26302
30MnCrTi4 1.8401 18ХГТ
30ХГТ
2 Approximate Comparison Table Structural Alloy Steel
China United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB SAE ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
15CrMn
16MnCr
20CrMnTi
5115 16MnCr5 16MnCr5 16MC5 16MnCr5 1.7131 18KHG 2127 527M17
590M17
3 Approximate Comparison Table Structural Alloy Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia
GB JIS SAE ISO W-Nr. NF EN/NF EN Numerical Grade GOST