Grade A1050AP
1050A
Corresponding Standard JIS H 4000-2022
Aluminium and aluminium alloy sheets, strips and plates
Classification Aluminum and Aluminum Alloys
A1050AP Chemical Element Composition Content (%)
Component Fe Si Mn Cu Ti V Al Zn Mg Other Individual
Minimum Value - - - - - - 99.5 - - -
Maximum Value 0.4 0.25 0.05 0.05 0.05 0.05 - 0.07 0.05 0.03
A1050AP Mechanical Properties
thickness
t
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
0.2≤t≤0.5 A1050AP-O O 65~95 ≥20 ≥20
0.5<t≤1.5 65~95 ≥20 ≥22
1.5<t≤3.0 65~95 ≥20 ≥26
3.0<t≤6.0 65~95 ≥20 ≥29
6<t≤12.5 65~95 ≥20 ≥35
12.5<t≤25 65~95 ≥20 ≥32
0.2≤t≤0.5 A1050AP-H14 H14 105~145 ≥85 ≥2
0.5<t≤1.5 105~145 ≥85 ≥3
1.5<t≤3.0 105~145 ≥85 ≥4
3.0<t≤6.0 105~145 ≥85 ≥5
0.2≤t≤0.5 A1050AP-H24 H24 105~145 ≥75 ≥3
0.5<t≤1.5 105~145 ≥75 ≥4
1.5<t≤3.0 105~145 ≥75 ≥5
3.0<t≤6.0 105~145 ≥75 ≥8
0.2≤t≤0.5 A1050AP-H18 H18 ≥140 ≥120 ≥1
0.5<t≤1.5 ≥140 ≥120 ≥2
1.5<t≤3.0 ≥140 ≥120 ≥2
Approximate Comparison Table Wrought Aluminum and Aluminum Alloy
China Japan United States International Organization for Standardization France European Standard Russia
GB JIS ASTM UNS ISO Numerical Grade NF EN/NF EN GOST
1050A 1050A
A91050
1050A A91050 Al99.5(A) A91050 A5
1050A
A91050
EN-AW-Al99.5(A) АД0/1011

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!