Grade 12Cr1MoVG
China ISC A31128
Corresponding Standard GB /T 5310-2023
Seamless steel tubes and pipes for high pressure boiler
Classification Alloy Steel
12Cr1MoVG Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value 0.08 0.17 0.4 - - 0.9 - - 0.25 0.15
Maximum Value 0.15 0.37 0.7 0.025 0.01 1.2 0.3 0.2 0.35 0.3
• total aluminum content Alt in the table.
• Unless required for smelting, elements not mentioned in this table should not be intentionally added to the steel without the purchaser\'s consent. The manufacturer shall take all appropriate measures to prevent elements that could impair the mechanical properties and suitability of the steel from being introduced through scrap or other materials used in the production process.
12Cr1MoVG Mechanical Properties
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
S ≤ 30mm Pipe
Normalizing + Tempering:
Normalizing Temperature 980~1020°C,
Tempering Temperature 720~760°C
S > 30mm Pipe
Quenching + Tempering or
Normalizing* + Tempering:
Quenching Temperature 950~990°C,
Tempering Temperature
470~640 or ReL
≥255
long. ≥21
tr. ≥19
HBW:135~195
HV:140~205
long. ≥40
tr. ≥27
• long.=Longitudinal;tr.=transverse;ReL=Lower yield strength
• For high-quality carbon steel and alloy steel pipes with D ≥ 76 mm and S ≥ 14 mm, impact tests shall be conducted. The impact absorption energy values listed in the table refer to the requirements for full-size Charpy V-notch specimens. When using sub-sized impact specimens, the minimum Charpy V-notch impact absorption energy requirements for 10 × 7.5 or 10 × 5 specimens shall be reduced to 0.75 or 0.5 times the full-size specimen requirements, respectively.
• The hardness testing of steel pipes shall comply with the following provisions:
ⓐ For steel pipes with S ≥ 5.0 mm, Brinell hardness test or Rockwell hardness test shall be conducted;
ⓑ For steel pipes with S < 5.0 mm, Rockwell hardness test shall be conducted (if Rockwell hardness values are not specified in the table, this test is not required);
ⓒ Upon the purchaser’s request, through mutual agreement between supplier and purchaser, and as specified in the contract, Vickers hardness test may be performed in place of Brinell or Rockwell hardness tests. When Vickers hardness testing of steel pipes is specified in the contract, the values shall meet the requirements given in the table.
• According to the buyer\'s request, and upon mutual agreement between the supplier and the buyer, with notation in the contract, a hardness test may be conducted on the outer surface of the steel pipe, and the values should comply with the specifications listed in the table.
12Cr1MoVG Corresponding Standards(Same grade name, different standards)