USA UNS S83071
Corresponding Standard ASTM A789/A789M-2024
Seamless and Welded Ferritic/Austenitic Stainless Steel Tubing for General Service
Classification Duplex Stainless Steel
Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - 0.5 - - 29 6 - 3 0.28
Maximum Value 0.03 0.5 1.5 0.03 0.02 31 8 0.8 4 0.4
Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Tube Solution heat treatment 1000~1150°C, rapid cooling by water or other methods ≥830 ≥680 ≥25 HBW: ≤300
HRC: ≤32
HV: ≤300*

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!