Grade SUS 305J1
Corresponding Standard JIS G 4315-2000
Stainless steel wires for cold heading and cold forging
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
SUS 305J1 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni
Minimum Value - - - - - 16.5 11
Maximum Value 0.08 1 2 0.045 0.03 19 13.5
SUS 305J1 Mechanical Properties
diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Wire WSA; 0.8≤d<2.0 Solid Solution After Drawing 530~680 ≥30 ≥70
Wire WSA; 0.8 ≤ d < 5.5 Solid Solution After Drawing 490~640 ≥40 ≥70
Wire WSB; 0.8≤d<2.0 Solid Solution After Drawing 560~740 ≥20 ≥65
Wire WSB; 2≤d≤17 Solid Solution After Drawing 510~690 ≥25 ≥65
Approximate Comparison Table Austenitic Stainless Steel
Japan United States France European Standard Russia United Kingdom
JIS ASTM NF EN/NF EN Numerical Grade GOST BS EN/BS
SUS305J1 305 Z1CN18-12
Z5CN18-11FF
X4CrNi18-12 1.4303 06KH18N11 305S19