Grade X2CrNiN18-10
Germany W-Nr. 1.4311
Corresponding Standard DIN EN 10296-2-2006
Welded circular steel tubes for mechanical and general engineering purposes — Technical delivery conditions — Part 2 Stainless steel
Classification Austenitic Stainless Steel
X2CrNiN18-10 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 17 8.5 0.12
Maximum Value 0.03 1 2 0.045 0.015 19.5 11.5 0.22
① a controlled sulfur content of 0,015% to 0,030% is specified.
X2CrNiN18-10 Mechanical Properties
condition Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Steel pipe: ≥550 Rp0.2:≥270
Rp1.0:≥305
l:≥35
t:≥30
◎ l=longitudinal, t=transverse
◎ Resistance to intergranular corrosiona: Yes (When tested in accordance with EN ISO3651-2)
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Sweden United Kingdom
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade SS BS EN/BS
022Cr19Ni10N
(00Cr18Ni10N)
S30453 304LN SUS 304LN STS 304LN 304LN S30453 X2CrNiN 18-9
X2CrNiN18-10
X2CrNiN 18-10 1.4311 Z2CN 18-1Az
Z3CN18-10Az
X2CrNiN 18-10 1.4311 2371 304S62
304S61