Grade X9CrNiSiNCe21-11-2
European Standard Steel Grade 1.4835
Corresponding Standard EN 10296-2-2005
Welded circular steel tubes for mechanical and general engineering purposes — Technical delivery conditions — Part 2 Stainless steel
Classification Austenitic Stainless Steel
X9CrNiSiNCe21-11-2 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N Ce
Minimum Value 0.05 1.4 - - - 20 10 0.12 0.03
Maximum Value 0.12 2.5 1 0.045 0.015 22 12 0.2 0.08
X9CrNiSiNCe21-11-2 Mechanical Properties
condition Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Steel pipe: ≥650 Rp0.2:≥310
Rp1.0:≥350
l:≥40;t:≥40
◎ l=longitudinal, t=transverse
◎ Elongation 20% min for wall thickness ≤35 mm after cold deformation.
1 Approximate Comparison Table Austenitic Stainless Steel
United States International Organization for Standardization European Standard
ASTM UNS ISO Numerical Grade Numerical Grade
F 45 S30815 X7CrNiSiNCe 21-11 4835-308-15-U 1.4835
2 Approximate Comparison Table Austenitic Heat-Resistant Steel
United States International Organization for Standardization European Standard Sweden
UNS ISO EN Numerical Grade SS
S30815 X7CrNiSiNCe21-11 X9CrNiSiNCe21-11-2 1.4835 2368