Grade Ni30
Corresponding Standard GB /T 12773-2021
Valve Steel and Superalloy Bars for Internal Combustion Engines
Classification Nickel and Nickel Alloys
Ni30 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo Ti Nb B Al More
Minimum Value - - - - - 13.5 29.5 - 0.4 2.3 0.4 - 1.6 Fe:Remainder
Maximum Value 0.08 0.5 0.5 0.015 0.015 15.5 33.5 0.2 1 2.9 0.9 0.01 2.2
Ni30 Mechanical Properties
condition Test Temperature Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
Hardness
HBW
Sample d=25 Room Temperature 900~1100°C Solution treated + 700~800°C×6h Air cooling ≥1000 Rp0.2: ≥600 ≥12 ≥30 ≥28HRC
Bar or Coil Room Temperature Solution treated ≤350
sample Solution treated + Aging High temperature short-term tensile strength 1030 High temperature short-term yield strength 640
sample Solution treated + Aging High temperature short-term tensile strength 1005 High temperature short-term yield strength 640
sample Solution treated + Aging High temperature short-term tensile strength 1000 High temperature short-term yield strength 640
sample Solution treated + Aging High temperature short-term tensile strength 950 High temperature short-term yield strength 670
sample Solution treated + Aging High temperature short-term tensile strength 900 High temperature short-term yield strength 680
sample Solution treated + Aging High temperature short-term tensile strength 650 High temperature short-term yield strength 565
sample Solution treated + Aging High temperature short-term tensile strength 540 -