Grade STS 403
Other Names
Corresponding Standard KS D 3697-2002
Stainless Steel Wires for Cold Heading and Cold Forging
Classification Martensitic Stainless Steel
STS 403 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni
Minimum Value - - - - - 11.5 -
Maximum Value 0.15 0.5 1 0.04 0.03 13 0.6
STS 403 Mechanical Properties
diameter or thickness
d
mm
Mark
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
Reduction of Area
ψ
%
0.8<d≤2 STS 403-WSB 540~740 - ≥65
2<d≤17 STS 403-WSB 460~640 ≥10 ≥65
Approximate Comparison Table Martensitic Stainless Steel
China Taiwan, China Japan South Korea United States Russia Sweden United Kingdom
GB ISC CNS JIS KS ASTM UNS GOST SS BS EN/BS
12Cr12
(1Cr12)
S40310 403 SUS 403 STS 403 403 S40300 08Х13 2301 403S17