Grade 416S41
Old Grade
Corresponding Standard BS 970-4-1970
Specification for Wrought steels in the form of blooms,billets,bars and forgings--Part 4:Valve steels
Classification Martensitic Stainless Steel
416S41 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo Se
Minimum Value 0.09 - - - - 11.5 - - - 0.15
Maximum Value 0.15 1 1.5 0.04 0.06 13.5 1 0.3 0.6 0.3
416S41 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
Steel, section≤152.4mm Hardened + tempered (P) 532~684 ≥334 ≥365 ≥15 152~207 Izod: ≥25ft·lbf
Steell, section≤63.5mm Hardened + tempered (R) 684~836 ≥486 ≥517 ≥11 201~255 Izod: ≥20ft·lbf
• The letters P, R, S and T in the table indicate the range of tensile strength of quenched and tempered steels.
• When supplied in the softened condition the hardness shall be 179 HB max.
416S41 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!