Grade CuCo2Be
European Standard Steel Grade CW104C
Corresponding Standard EN 12167-2024
Copper and copper alloys - Profiles and bars for general purposes
Classification Copper and Copper Alloys
Density 8.8 g/cm3
CuCo2Be Chemical Element Composition Content (%)
Component Fe Be Ni Co Other Total More
Minimum Value - 0.4 - 2 - Cumin:Rem.
Maximum Value 0.2 0.7 0.3 2.8 0.5
"Other individual elements or other totals": The chemical composition includes elements not specified in the table. Analysis should only be conducted if these elements are suspected to be present, or if routine analysis suggests that their content may exceed the prescribed limits.
CuCo2Be Mechanical Properties
thickness
t
mm
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
3≤t≤30 CuCo2Be-R730 R730 ≥730 ≥610 ≥2(A100), ≥4(A11.3), ≥8(A)
30≤t≤100 CuCo2Be-R680 R680 ≥680 ≥550 ≥10(A)
3≤t≤30 CuCo2Be-H230 H230 230~310
30≤t≤100 CuCo2Be-H220 H220 220~270
All specifications CuCo2Be-M M As manufactured As manufactured As manufactured As manufactured
Test pieces shall be in accordance with EN ISO 6892-1:2019, except that 200 mm gauge length is not permitted.
Elongation requirements for rod of thickness or diameter equivalent to the cross sectional area:
ⓐ less than 4 mm (A100 mm);
ⓑ 4 mm up to and including 8 mm (A 11,3);
ⓒ greater than 8 mm (A);
1 Approximate Comparison Table Processing of high copper alloy
China Japan United States International Organization for Standardization Germany European Standard Russia
GB ISC JIS ASTM UNS ISO Numerical Grade DIN EN/DIN W-Nr. EN Numerical Grade GOST
TBe0.6-2.5
QBe0.6-2.5
C17500 C1750
C17500
97Cu-.5Be-2.5Co C17500 CuCo2Be C17500 CuCo2Be C17500
2.1285
CuCo2Be CW104C БрБК0.6-2.5
2 Approximate Comparison Table Cupper and cupper alloy
Germany European Standard
DIN EN/DIN W-Nr. EN Numerical Grade
CuCo2Be 2.1285 CuCo2Be CW104C

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!