Grade X3CrNiMo13-4
European Standard Steel Grade 1.4313
Corresponding Standard EN 10272-2016
Stainless Steel Bars for Pressure Purposes
Classification Martensitic Stainless Steel
X3CrNiMo13-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 12 3.5 0.3 0.02
Maximum Value 0.05 0.7 1.5 0.04 0.015 14 4.5 0.7 -
X3CrNiMo13-4 Mechanical Properties
Diameter or thickness
d or b
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
≤160 +QT 650 700~800 ≥520 l: ≥15 l: ≥70 (at 20℃)
l: ≥40(at -20℃)
160<d (b)≤250 +QT 650 700~800 ≥520 tr: ≥14 tr: ≥50 (at 20℃)
≤160 +QT 780 780~980 ≥620 l: ≥15 l: ≥70 (at 20℃)
160<d (b)≤250 +QT 780 780~980 ≥620 tr: ≥14 tr: ≥50 (at 20℃)
≤160 +QT 900 900~1100 ≥800 l: ≥14 l: ≥50 (at 20℃)
160<d (b)≤250 +QT 900 900~1100 ≥800 tr: ≥14 tr: ≥40 (at 20℃)
a) Axial: l;Tangential:tr.
b) +QT= quenched and tempered.
1 Approximate Comparison Table Other Stainless Steels
Germany France European Standard Sweden United Kingdom
DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade SS BS EN/BS
X5CrNi 13-4 1.4313 Z25CN 13-4 X3CrNiMo 13-4 1.4313 2385 425C11
2 Approximate Comparison Table Martensitic Stainless Steel
China Japan United States International Organization for Standardization European Standard
GB ISC JIS UNS ISO EN Numerical Grade
04Cr13Ni5Mo S41595 SUS F6NM S41500 X3CrNiMo 13-4 X3CrNiMo 13-4 1.4313
3 Approximate Comparison Table Martensitic Stainless Steel
United States France European Standard Sweden
UNS NF EN/NF EN Numerical Grade SS
S41500 Z6CN13-04 X3CrNiMo13-4 1.4313 2385
4 Approximate Comparison Table Martensitic Stainless Steel
China European Standard
GB EN
0Cr13Ni5Mo X3CrNiMo13-4

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!