Grade X4CrNiMo16-5-1
European Standard Steel Grade 1.4418
Corresponding Standard EN 10272-2016
Stainless steel bars for pressure purposes
Classification Martensitic Stainless Steel
X4CrNiMo16-5-1 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 15 4 0.8 0.02
Maximum Value 0.06 0.7 1.5 0.04 0.015 17 6 1.5 -
① Particular ranges of sulfur content may provide improvement of particular properties. For machinability, a controlled sulfur content of 0,015 % to 0,030 % is recommended and may be agreed. For weldability, a controlled sulfur content of 0,008 % to 0,030 % is recommended and may be agreed.
X4CrNiMo16-5-1 Mechanical Properties
Diameter or thickness
d or b
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
≤160 +QT 760 760~960 ≥550 l: ≥16 l: ≥90 (at 20℃)
l: ≥40 (at -20℃)
160<d (b)≤250 +QT 760 760~960 ≥550 tr: ≥14 tr: ≥70 (at 20℃)
≤160 +QT 900 900~1100 ≥700 l: ≥16 l: ≥80 (at 20℃)
160<d (b)≤250 +QT 900 900~1100 ≥700 tr: ≥14 tr: ≥60 (at 20℃)
a) Axial: l;Tangential:tr.
b) +QT= quenched and tempered.
Approximate Comparison Table
International Organization for Standardization European Standard
ISO Numerical Grade EN Numerical Grade
X4CrNiMo16-5-1 4418-431-77-E X4CrNiMo16-5-1 1.4418