Grade C45EC
Germany W-Nr. 1.1192
Old Grade
Corresponding Standard DIN EN 10263-4-2002
Steel rod, bars and wire for cold heading and cold extrusion Part 4: Technical delivery conditions for steels for quenching and tempering
Classification Carbon Steel
Properties Forgability
C45EC Chemical Element Composition Content (%)
Component C Si Mn P S Cu
Minimum Value 0.42 - 0.5 - - -
Maximum Value 0.5 0.3 0.8 0.025 0.025 0.25
C45EC Mechanical Properties
diameter
d
mm
Tensile Strength
σb
Mpa
Elongation or Extension Rate
δ
%
2<d≤5 Conditioned type (cold-rolled delivery)
≤590
Nickel-chromium reduction of area Z%
≥62
5<d≤40 ≤580 ≥62
2<d≤5 Surface hardening type (cold-rolled delivery)
≤630
Nickel-chromium reduction of area Z%
≥60
5<d≤40 ≤620 ≥60
5<d≤40 Non-heat treated type (hot-rolled delivery)
≤600
Nickel-chromium reduction of area Z%
≥60
5<d≤10 Heat treated (cold-rolled delivery)
≤720
10<d≤40 ≤710
New and Old Grade Replacement List
Approximate Comparison Table
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France Russia
GB ISC CNS JIS KS ASTM/AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF GOST
ML45 U40452 SWRCH45K SWRCH45K SWRCH45K 1044 G10440 CE45E4
(C6)
Cq45
(C45C)
1.1192 XC45 45