Grade X1NiCrMoCuN25-20-7
European Standard Steel Grade 1.4529
Corresponding Standard EN 10272-2016
Stainless steel bars for pressure purposes
Classification Austenitic Stainless Steel
X1NiCrMoCuN25-20-7 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - - - - 19 24 0.5 6 0.15
Maximum Value 0.02 0.5 1 0.03 0.01 21 26 1.5 7 0.25
X1NiCrMoCuN25-20-7 Mechanical Properties
Diameter or thickness
d or b
mm
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
≤160 650~850 Rp0.2:≥300
Rp1.0:≥340
l: ≥40 ≤250 (at 20℃):l ≥100
(at -196℃):≥40
160<d (b)≤400 650~850 Rp0.2:≥300
Rp1.0:≥340
tr: ≥35 ≤250 (at 20℃):tr ≥60
(at -196℃):≥ 40
a) Axial: l;Tangential:tr.
* The maximum HBW-values may be raised by 100 units or the tensile strength value may be raised by 200 MPa and the minimum elongation value be lowered to 20 % for bars of ≤ 35 mm thickness having a final cold deformation.
1 Approximate Comparison Table
China United States International Organization for Standardization Germany European Standard
GB Commercial Grade UNS ISO Numerical Grade DIN EN/DIN W-Nr. EN Numerical Grade
25-6Mo Incoloy926 N08926 X1NiCrMoCuN25-20-7 4529-089-26-I X1NiCrMoCuN25-20-7 1.4529 X1NiCrMoCuN25-20-7 1.4529
2 Approximate Comparison Table
United States European Standard
ASTM EN Numerical Grade
N08926
NO8367
X1NiCrMoCuN25-20-7 1.4529

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!