Grade X1NiCrMoCu31-27-4
European Standard Steel Grade 1.4563
Corresponding Standard EN 10272-2016
Stainless Steel Bars for Pressure Purposes
Classification Austenitic Stainless Steel
X1NiCrMoCu31-27-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - - - - 26 30 0.7 3 -
Maximum Value 0.02 0.7 2 0.03 0.01 28 32 1.5 4 0.1
X1NiCrMoCu31-27-4 Mechanical Properties
Diameter or thickness
d or b
mm
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
≤160 500~750 Rp0.2:≥220
Rp1.0:≥250
l: ≥35 ≤230 (at 20℃):l ≥100
(at -196℃):≥60
160<d (b)≤400 500~750 Rp0.2:≥220
Rp1.0:≥250
tr: ≥30 ≤230 (at 20℃):tr ≥60
(at -196℃):≥ 60
a) Axial: l;Tangential:tr.
* The maximum HBW-values may be raised by 100 units or the tensile strength value may be raised by 200 MPa and the minimum elongation value be lowered to 20 % for bars of ≤ 35 mm thickness having a final cold deformation.
1 Approximate Comparison Table Corrosion-Resistant Alloy
China United States Germany
GB ISC UNS DIN EN/DIN W-Nr.
NS 1404
BG2830
H 08028 N 08028
Sanicro 28
X1NiCrMoCu 31-27-4 1.4563
2 Approximate Comparison Table Austenitic Stainless Steel
United States International Organization for Standardization European Standard
UNS ISO Numerical Grade EN Numerical Grade
N08028 X1NiCrMoCu31-27-4 4563-080-28-I X1NiCrMoCu31-27-4 1.4563