Grade P195GH
European Standard Steel Grade 1.0348
Corresponding Standard EN 10217-2-2019
Part 2: Electric Welded Non-Alloy and Alloy Steel Tubes with Specified Elevated Temperature Properties
Classification Carbon Steel
P195GH Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo Ti * V * Nb * Al More
Minimum Value - - - - - - - - - - - - 0.02 Cr+Cu+Mo+Ni≤0.7
Maximum Value 0.13 0.35 0.7 0.025 0.02 0.3 0.3 0.3 0.08 0.03 0.02 0.01 -
* The content of these elements need not to be reported unless intentionally added to the cast.
※ In order to facilitate subsequent forming operations, an agreed maximum copper content lower than indicated and an agreed specified maximum tin content shall apply
◎ For Al/N ratios ≥ 2, if nitrogen is fixed by niobium, titanium or vanadium, details of which shall be reported, this requirement does not apply except that when using titanium, the steel producer shall verify that (Al+Ti/2) ≥ 0,020 %.
P195GH Mechanical Properties
wall thickness
T
mm
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
T≤16 320~440 or ReH
≥195
≥27(l)
≥25(t)
0°C:
≥40(l);≥27(t)
-10°C: ≥28(l)
• l = longitudinal t = transverse
P195GH Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!