Grade X1NiCrMoCu 31-27-4
European Standard Steel Grade 1.4563
Corresponding Standard EN 10217-7-2021
Part 7: Stainless steel tubes
Classification Austenitic Stainless Steel
X1NiCrMoCu 31-27-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N
Minimum Value - - - - - 26 30 0.7 3 -
Maximum Value 0.02 0.7 2 0.03 0.01 28 32 1.5 4 0.1
X1NiCrMoCu 31-27-4 Mechanical Properties
wall thickness
T
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
T≤60 Solution annealing (+AT) 500~750 ≥215 Rp1.0
≥245
≥40(l)
≥35(t)
室温
≥120(l);≥90(t)
-196°C
≥60(t)
• l=longitudinal;t=transverse
• Solution annealing temperature: 1100-1160°C, rapid cooling in water and air.Resistant to intergranular corrosion. Method C in EN ISO 3651-2-1998.
1 Approximate Comparison Table Corrosion-Resistant Alloy
China United States Germany
GB ISC UNS DIN EN/DIN W-Nr.
NS 1404
BG2830
H 08028 N 08028
Sanicro 28
X1NiCrMoCu 31-27-4 1.4563
2 Approximate Comparison Table Austenitic Stainless Steel
United States International Organization for Standardization European Standard
UNS ISO Numerical Grade EN Numerical Grade
N08028 X1NiCrMoCu31-27-4 4563-080-28-I X1NiCrMoCu31-27-4 1.4563

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!