Grade X2CrNiMoCuWN 25-7-4
European Standard Steel Grade 1.4501
Corresponding Standard EN 10217-7-2021
Part 7: Stainless steel tubes
Classification Duplex Stainless Steel
X2CrNiMoCuWN 25-7-4 Chemical Element Composition Content (%)
Component C Si Mn P * S * Cr Ni Cu Mo N W
Minimum Value - - - - - 24 6 0.5 3 0.2 0.5
Maximum Value 0.03 1 1 0.035 0.015 26 8 1 4 0.3 1
* For tubes welded without filler material the sum of sulphur and phosphorus shall be maximum 0,040 %.
X2CrNiMoCuWN 25-7-4 Mechanical Properties
wall thickness
T
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
T≤30 Solution annealing (+AT) 800~1000 ≥550 ≥20(l)
≥20(t)
室温
≥100(l);≥100(t)
-40°C
≥40(t)
• l=longitudinal;t=transverse
• Solution annealing temperature: 1080-1160°C, rapid cooling in water and air. Resistant to intergranular corrosion. Method B or C in EN ISO 3651-2-1998.
1 Approximate Comparison Table Austenitic-Ferritic Stainless Steel
China Japan United States International Organization for Standardization Germany European Standard
GB ISC JIS UNS ISO DIN EN/DIN W-Nr. EN Numerical Grade
022Cr25Ni7Mo4WCuN
00Cr23Ni7Mo3.5WCuN*
S27603 SUS329J2L S32760 X2CrNiMoCuWN 25-7-4 X2CrNiMoCuWN 25-7-4 1.4501 X2CrNiMoCuWN 25-7-4 1.4501
2 Approximate Comparison Table Austenitic-Ferritic Stainless Steel
China Japan United States Germany European Standard
GB JIS UNS DIN EN/DIN W-Nr. EN Numerical Grade
00Cr23Ni7Mo3.5WCuN SUS329J2L S32750
S32760
X2CrNiMoCuWN25-7-4 1.4501 X2CrNiMoCuWN25-7-4 1.4501

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!