Grade SA537 Class 1
Corresponding Standard ASME SA-537/SA-537M-2023
Pressure Vessel Plates, Heat-Treated, Carbon-Manganese- Silicon Steel
Classification Alloy Steel
SA537 Class 1 Chemical Element Composition Content (%)
  Component C Si Mn * P S Cr Ni * Cu Mo
厚度≤1-1/2in.(40mm) Minimum Value - 0.15 0.7 - - - - - -
Maximum Value 0.24 0.5 1.35 0.025 0.025 0.25 0.25 0.35 0.08
  Component C Si Mn P S Cr Ni * Cu Mo
厚度>1-1/2in.(40mm) Minimum Value - 0.15 1 - - - - - -
Maximum Value 0.24 0.5 1.6 0.025 0.025 0.25 0.25 0.35 0.08
* Manganese may exceed 1.35 % on heat analysis, up to a maximum of 1.60 %, and nickel may exceed 0.25 % on heat analysis, up to a maximum of 0.50 %, provided the heat analysis carbon equivalent does not exceed 0.57 % when based upon the following equation: CE=C+Mn/6+(Cr+Mo+V)/5+(Ni+Cu)/15
SA537 Class 1 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
t≤65 Normalizing 485~620 ≥345 ≥22
65<t≤100 Normalizing 450~585 ≥310 ≥22
t>100 Normalizing 450~585 ≥310 ≥22

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!