Grade X8Ni9
European Standard Steel Grade 1.5662
Corresponding Standard EN 10028-4-2017
Flat Products Made of Steels for Pressure Purposes - Part Four: Nickel Alloy Steels with Specified Low Temperature Properties
Classification Alloy Steel
X8Ni9 Chemical Element Composition Content (%)
Component C Si Mn P S Ni Mo V More
Minimum Value - - 0.3 - - 8.5 - - Cr+Cu+Mo≤0.50
Maximum Value 0.1 0.35 0.8 0.02 0.005 10 0.1 0.05
X8Ni9 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
t≤30 Normalizing (+N) + Normalizing and tempering (+NT) 640~840 ReH
≥490
≥18
30<t≤50 Normalizing (+N) + Normalizing and tempering (+NT) 640~840 ReH
≥480
≥18
t≤30 Qenching + tempering (+QT) 640~840 ReH
≥490
≥18
30<t≤125 Qenching + tempering (+QT) 640~840 ReH
≥480
≥18
t≤30 Qenching + tempering (+QT) 680~820 ReH
≥585
≥18
30<t≤125 Qenching + tempering (+QT) 680~820 ReH
≥575
≥18
Approximate Comparison Table Pressure-Bearing Flat Steel
China Japan United States International Organization for Standardization European Standard
GB JIS ASTM ISO EN
06Ni9DR
GB/T 713.4-2023
SL9N590
JIS G 3127-2021
9%Ni
ASTM A533/A533M-17
X7Ni9
ISO 9328-4-2018
X8Ni9
X7Ni9
EN 10028-4-2017