Grade 25CrMo4
Corresponding Standard JIS G 7105-2000
Heat-Treatable Steels, Alloy Steels and Free-Cutting Steels — Part 18 : Bright Products Of Unalloyed and Low Alloy Steels
Classification Alloy Steel
Properties Carburizing Ability
25CrMo4 Chemical Element Composition Content (%)
Component C Si * Mn P S Cr Mo
Minimum Value 0.22 0.1 0.6 - - 0.9 0.15
Maximum Value 0.29 0.4 0.9 0.035 0.035 1.2 0.3
◎ Steels with machinability which has been improved either by the addition of lead or by higher sulfur levels up to about 0.100 % (m/m) S (including controlled sulfide morphology) may be available on request.
* Steels may be supplied with a lower silicon content, in which case alternative means of deoxidation must be used.
25CrMo4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Impact Energy Absorption
KV2
J
t≤16 TC ≤880
16<t≤40 TC ≤860
40<t≤80 TC ≤840
t≤80 TC+TA,
P+TA
or
G+TA
≤212
t≤16 TC+TQ+TT℗,
P+TQ+TT
or
G+TQ+TT
900~1100 ≥700 ≥12 KU: ≥30
KV: ≥45
16<t≤40 TC+TQ+TT℗,
P+TQ+TT
or
G+TQ+TT
800~950 ≥600 ≥14 KU: ≥35
KV: ≥50
40<t≤80 TC+TQ+TT℗,
P+TQ+TT
or
G+TQ+TT
700~850 ≥450 ≥15 KU: ≥35
KV: ≥50

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!