Grade X3CrNiMoBN17-13-3
European Standard Steel Grade 1.4910
Corresponding Standard EN 10269-2006
Steels and nickel alloys for fasteners with specified elevated and/or low temperature properties
Classification Austenitic Stainless Steel
Properties Corrosion Resistance
Density 8 g/cm3
X3CrNiMoBN17-13-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N B
Minimum Value - - - - - 16 12 2 0.1 0.0015
Maximum Value 0.04 0.75 2 0.035 0.015 18 14 3 0.18 0.005
①Elements not listed in this table may not be intentionally added to the steel without the agreement of the purchaser except for finishing the cast. All appropriate precautions are to be taken to avoid the addition of such elements from scrap and other materials used in production which would impair mechanical properties and the usefulness of the steel.
X3CrNiMoBN17-13-3 Mechanical Properties
diameter
d
mm
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
d≤160 Solid Solution Annealing (+AT)
550~750
Solid Solution Annealing (+AT)
≥260
Lo = 5.65√So
≥35
①+AT = solution annealed; +C = cold work hardened; +N = normalized; +NT = normalized and tempered; +P = precipitation hardened; +QT = quenched and tempered; WW = Warm worked.
Approximate Comparison Table
International Organization for Standardization European Standard
ISO Numerical Grade EN Numerical Grade
X3CrNiMoBN 17-13-3 4910-316-77-E X3CrNiMoBN 17-13-3 1.4910