Grade 17-7PH
Corresponding Standard SAE AMS 5528H-2007
Steel, Corrosion-Resistant, Sheet, Strip, and Plate 17Cr - 7.1Ni - 1.1Al Solution Heat Treated, Precipitation Hardenable
Classification Other Stainless Steels
Properties Corrosion Resistance
17-7PH Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Al
Minimum Value - - - - - 16 6.5 0.75
Maximum Value 0.09 1 1 0.04 0.03 18 7.75 1.5
17-7PH Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
0.13<t≤0.25 Solution Heat Treatment (S) ≤1034 ≤448 ≥20 HRB
≤92
t>0.25 Solution Heat Treatment (S) ≤1034 ≤379 ≥20 ≤92
0.13<t≤0.25 TH1050 1241~1448 ≥1035 ≥4 HRC
38~46
0.25<t≤0.48 TH1050 1241~1448 ≥1035 ≥5 38~46
0.48<t≤25.4 TH1050 1241~1448 ≥1035 ≥6 38~46
Approximate Comparison Table Precipitation Hardening Stainless Steel
China United States
GB SAE
0Cr17Ni7Al 17-7PH
17-7PH Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!