Grade X12Ni5
European Standard Steel Grade 1.5680
Corresponding Standard EN 10216-4-2013
Seamless Steel Tubes For Pressure Purpose - Technical Delivery Condition - Part 4: Non-Alloy and Alloy Steel Tubes with Specified Low Temperature Properties
Classification Carbon Steel
X12Ni5 Chemical Element Composition Content (%)
Component C Si Mn P S Ni Cu V
Minimum Value - - 0.3 - - 4.5 - -
Maximum Value 0.15 0.35 0.8 0.02 0.005 5.3 0.3 0.05
X12Ni5 Mechanical Properties
wall thickness
T
mm
Test Temperature Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
T≤40 Room Temperature 510~710 ReH or Rp0.2
≥390
l: ≥21
t: ≥19
l: ≥70
t: ≥50
/ T≤25
l: ≥70
t: ≥50
25<T≤40
l: ≥65
t: ≥45
/ T≤25
l: ≥65
t: ≥45
25<T≤40
l: ≥65
t: ≥45
/ T≤25
l: ≥65
t: ≥45
25<T≤40
l: ≥65
t: ≥45
/ T≤25
l: ≥65
t: ≥45
25<T≤45
l: ≥60
t: ≥40
/ T≤25
l: ≥55
t: ≥35
25<T≤45
l: ≥50
t: ≥30
/ T≤25
l: ≥50
t: ≥30
25<T≤45
l: ≥45
t: ≥30
/ T≤25
l: ≥45
t: ≥30
25<T≤45
l: ≥40
t: ≥27
/ T≤25
l: ≥40
t: ≥27
• l=longitudinal;t=transverse
Approximate Comparison Table Pressure-Bearing Flat Steel
China Japan International Organization for Standardization European Standard
GB JIS ISO EN
07Ni5DR
GB/T 713.4-2023
SL5N590
JIS G 3127-2021
X12Ni5
ISO 9328-4-2018
X12Ni5
EN 10028-4-2017

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!