Grade X2CrNiN18-7
European Standard Steel Grade 1.4318
Corresponding Standard EN 10028-7-2016
Flat Products Made of Steels for Pressure Purposes - Part 7: Stainless Steels
Classification Austenitic Stainless Steel
X2CrNiN18-7 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni N
Minimum Value - - - - - 16.5 6 0.1
Maximum Value 0.03 1 2 0.045 0.015 18.5 8 0.2
X2CrNiN18-7 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
C:T ≤ 8 +AT 650~850 tr©.
Rp0.2:≥350
Rp1.0:≥380
T<3mm, A80①
long.+tr. :≥35©;
T≥3mm, A②
long.+tr. :≥40©
20°C
long.: ≥90; tr.: ≥60
-196°C
tr.: ≥60
H:T ≤ 13.5 +AT 650~850 tr©.
Rp0.2:≥330
Rp1.0:≥370
T<3mm, A80①
long.+tr. :≥35©;
T≥3mm, A②
long.+tr. :≥40©
20°C
long.: ≥90; tr.: ≥60
-196°C
tr.: ≥60
P:T ≤ 75 +AT 650~850 tr©.
Rp0.2:≥330
Rp1.0:≥370
T<3mm, A80①
long.+tr. :≥35©;
T≥3mm, A②
long.+tr. :≥40©
20°C
long.: ≥90; tr.: ≥60
-196°C
tr.: ≥60
• C=cold rolled strip;H=hot rolled strip;P=hot rolled plate
• +A=Annealed;+AT=Solution annealed
• B=width;T=thick
1 Approximate Comparison Table Austenitic Stainless Steel
China Japan United States International Organization for Standardization European Standard
ISC JIS ASTM UNS ISO Numerical Grade EN Numerical Grade
S30153 SUS 301L 301LN S30153 X2CrNiN18-7 4318-301-53-I X2CrNiN18-7 1.4318
2 Approximate Comparison Table Austenitic Stainless Steel
Japan United States France European Standard
JIS ASTM NF EN/NF EN Numerical Grade
SUS301L 301LN Z3CN18-07Az X2CrNiN18-7 1.4318