Grade X2CrNiMo18-14-3
European Standard Steel Grade 1.4435
Corresponding Standard EN 10028-7-2016
Flat Products Made of Steels for Pressure Purposes - Part 7: Stainless Steels
Classification Austenitic Stainless Steel
X2CrNiMo18-14-3 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Mo N
Minimum Value - - - - - 17 12.5 2.5 -
Maximum Value 0.03 1 2 0.045 0.015 19 15 3 0.1
X2CrNiMo18-14-3 Mechanical Properties
condition Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
C:T ≤ 8 +AT 550~700 tr©
Rp0.2:≥240
Rp1.0:≥270
T<3mm, A80①
long.+tr. :≥40;
T≥3mm, A②
long.+tr. :≥40
©
20°C
long.: ≥100
tr.: ≥60
-196°C
tr.: ≥60
H:T ≤ 13.5 +AT 550~700 tr©
Rp0.2:≥220
Rp1.0:≥260
T<3mm, A80①
long.+tr. :≥40;
T≥3mm, A②
long.+tr. :≥40
©
20°C
long.: ≥100
tr.: ≥60
-196°C
tr.: ≥60
P:T ≤ 75 +AT 520~670 tr©
Rp0.2:≥220
Rp1.0:≥260
T<3mm, A80①
long.+tr. :≥45;
T≥3mm, A②
long.+tr. :≥45
©
20°C
long.: ≥100
tr.: ≥60
-196°C
tr.: ≥60
• C=cold rolled strip;H=hot rolled strip;P=hot rolled plate
• +A=Annealed;+AT=Solution annealed
• B=width;T=thick
Approximate Comparison Table Austenitic Stainless Steel
China Japan United States International Organization for Standardization Germany France European Standard Russia Sweden United Kingdom
GB JIS ASTM ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST SS BS EN/BS
00Cr17Ni14Mo2 SUS316L 316L
TP316L
Type19a X2CrNiMo18-14-3 Z3CND17-12-03
Z3CND18-14-03
X2CrNiMo18-14-3 1.4435 03KH17N14M3 2353 316S13
316S14