Grade 34Cr4
Corresponding Standard ISO 683-1-1987
Heat-Treatable Steels,alloy Steels and Free-Cutting Steels. Part 1:Direct-Hardening Unalloyed and Low-Alloyed Wrought Steel in Form of Different Black Produts
Classification Alloy Steel
34Cr4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr
Minimum Value 0.3 0.1 0.6 - - 0.9
Maximum Value 0.37 0.4 0.9 0.035 0.035 1.2
• The designations are in accordance with the system proposed by ISO/TC 17/SC 2.
• Elements not quoted should not be intentionally added to the steel without the agreement of the purchaser, other than for the purpose of finishing the heat. All reasonable precautions should be taken to prevent the addition, from scrap or other material used in manufacture, of such elements which affect the hardenability, mechanical properties and applicability.
• In the case of the grades with specified hardenability requirements (see tables 5 to 7), except for phosphorous and sulfur, insignificant deviations from the limits for cast analysis are permissible; these deviations shall, however, not exceed in the case of carbon ± 0,01 % (m/m) and in all other cases the values according to table 4.
• For boron-treated steels, see ISO 4954.
• Steels with improved machinability by either lead additions or higher sulfur levels up to about 0,100 % (m/m) S (including controlled sulfide morphology) may be available on request.
34Cr4 Mechanical Properties
thickness
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
d≤16 Qenching + tempering 900~1100 ≥700 ≥12 KU
≥25
16<d≤40 Qenching + tempering 800~950 ≥590 ≥14 KU
≥30
40<d≤100 Qenching + tempering 700~850 ≥460 ≥15 KU
≥30
1 Approximate Comparison Table Structural Alloy Steel
China Taiwan, China Japan South Korea United States International Organization for Standardization Germany France European Standard Russia United Kingdom
GB ISC CNS JIS KS ASTM/AISI UNS ISO DIN EN/DIN W-Nr. NF EN/NF EN Numerical Grade GOST BS EN/BS
35Cr A20352 SCr435 SCr435
SCr435H
SCr435 5135 G51350 34Cr4 34Cr4 1.7033 38C4 34Cr4 1.7033 35Х 530A36
2 Approximate Comparison Table Structural Alloy Steel
Japan International Organization for Standardization Germany France European Standard Russia United Kingdom
JIS ISO DIN EN/DIN NF EN/NF EN Numerical Grade GOST BS EN/BS
SCr430H 34Cr4 34Cr4 32C4 34Cr4 1.7033 30KH
35KH
530H32
530M32
3 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
Japan International Organization for Standardization European Standard
JIS ISO EN Numerical Grade
SCr435
SCr435H
34Cr4 34Cr4 1.7033
4 Approximate Comparison Table Steel for Cold Heading and Cold Extrusion
China Japan United States International Organization for Standardization European Standard
GB JIS ASTM/AISI ISO EN
ML35Cr SCr435 5135 34Cr4 34Cr4

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!