Grade SA335 Grade P36
K21001
Corresponding Standard ASME SA-335/SA-335M-2021
Standard Specification for Seamless Ferritic Alloy-Steel Pipe for High-Temperature Service
Classification Alloy Steel
SA335 Grade P36 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo N V Al Cb
Minimum Value 0.1 0.25 0.8 - - - 1 0.5 0.25 - - - 0.015
Maximum Value 0.17 0.5 1.2 0.03 0.025 0.3 1.3 0.8 0.5 0.02 0.2 0.05 0.045
SA335 Grade P36 Mechanical Properties
Mark
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
Hardness
HBW
Class 1 Normalizing(≥900°C) + Tempering(≥595°C) ≥415 ≥205 l: ≥15 HBW: ≤250
HV: ≤265
HRC: ≤25
Class 2 cooled from the austenitizing temperature by accelerated cooling in air or by liquid quenching ≥660 ≥460 l: ≥15

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!