Grade SUS315J1TB
Corresponding Standard JIS G 3463-2012
Stainless Steel Boiler and Heat Exchanger Tubes
Classification Austenitic Stainless Steel
SUS315J1TB Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo
Minimum Value - 0.5 - - - 17 8.5 0.5 0.5
Maximum Value 0.08 2.5 2 0.045 0.03 20.5 11.5 3.5 1.5
• When the customer requests product analysis, the carbon content shall be limited ≤ 0.035%
SUS315J1TB Mechanical Properties
outside diameter
d
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Yield Point
σs
Mpa
Elongation or Extension Rate
δ
%
d<10 ST ≥520 ≥205 ≥27
10≤d<20 ST ≥520 ≥205 ≥30
d≤20 ST ≥520 ≥205 ≥35
SUS315J1TB Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!