Grade G35CrNiMo6-6
ISO Numeric Designation 1.6579
Corresponding Standard ISO 14737-2021
Carbon and Low Alloy Cast Steels for General Applications
Classification Cast Steel
G35CrNiMo6-6 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value 0.32 - 0.6 - - 1.4 1.4 - 0.15 -
Maximum Value 0.38 0.6 1 0.025 0.02 1.7 1.7 0.3 0.35 0.05
① For castings of ruling thickness < 28 mm, S ≤ 0,030 % is permitted.
G35CrNiMo6-6 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤150 Normalizing (+N),860~920℃ 800~950 ≥550 ≥12 ≥31
150<t≤250 Normalizing (+N),860~920℃ 750~900 ≥500 ≥12 ≥31
t≤100 Quenching + Tempering (+QT1)
Quenching temperature 860~920°C , Tempering temperature 600~650°C
850~1000 ≥700 ≥12 ≥45
100<t≤150 Quenching + Tempering (+QT1)
Quenching temperature 860~920°C , Tempering temperature 600~650°C
800~950 ≥650 ≥12 ≥35
150<t≤250 Quenching + Tempering (+QT1)
Quenching temperature 860~920°C , Tempering temperature 600~650°C
800~950 ≥650 ≥12 ≥30
t≤100 Quenching + Tempering (+QT2)
Quenching temperature 860~920°C , Tempering temperature 510~560°C
900~1050 ≥800 ≥10 ≥35
G35CrNiMo6-6 Corresponding Standards(Same grade name, different standards)