Grade A681 Type H19
USA UNS T20819
AISI
American Iron and Steel Institute
H19
Corresponding Standard ASTM A681-2024
Tool Steels Alloy
Classification Tool Steel
A681 Type H19 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Mo W V Co More
Minimum Value 0.32 0.15 0.2 - - 4 0.3 3.75 1.75 4 Ni+Cu≤0.75
Maximum Value 0.45 0.5 0.5 0.03 0.03 4.75 0.55 4.5 2.2 4.5
A681 Type H19 Mechanical Properties
condition Heat Treatment or Condition
Hardness
HBW
condition of delivery Cold Drawing BHN
≤262
condition of delivery Annealing BHN
≤241
specimen Preheat at 788±14 ℃, heat at 1191±5.6℃(controlled atmosphere) or 1177℃(salt bath), hold for 5 to 15 min air cool. Temper twice at 552±5.6℃, each time for 2 h HRC
≥55
A681TypeH19 Corresponding Standards(Same grade name, different standards)