Grade A681 Type H25
USA UNS T20825
AISI
American Iron and Steel Institute
H25
Corresponding Standard ASTM A681-2024
Tool Steels Alloy
Classification Tool Steel
A681 Type H25 Chemical Element Composition Content (%)
Component C Si Mn P S Cr W V More
Minimum Value 0.22 0.15 0.15 - - 3.75 14 0.4 Ni+Cu≤0.75
Maximum Value 0.32 0.4 0.4 0.03 0.03 4.5 16 0.6
A681 Type H25 Mechanical Properties
condition Heat Treatment or Condition
Hardness
HBW
condition of delivery Cold Drawing BHN
≤262
condition of delivery Annealing BHN
≤235
specimen Preheat at 788±14 ℃, heat at 1246±5.6℃(controlled atmosphere) or 1232℃(salt bath), hold for 5 to 15 min,air cool. Temper twice at 552±5.6℃, each time for 2 h HRC
≥44
A681TypeH25 Corresponding Standards(Same grade name, different standards)