Grade A681 Type H42
USA UNS T20842
AISI
American Iron and Steel Institute
H42
Corresponding Standard ASTM A681-2024
Tool Steels Alloy
Classification Tool Steel
A681 Type H42 Chemical Element Composition Content (%)
Component C * Si Mn P S Cr Mo W V More
Minimum Value 0.5 0.2 0.15 - - 3.75 4.5 5.5 1.75 Ni+Cu≤0.75
Maximum Value 0.7 0.45 0.4 0.03 0.03 4.5 5.5 6.75 2.2
*Available in several carbon ranges.
A681 Type H42 Mechanical Properties
condition Heat Treatment or Condition
Hardness
HBW
condition of delivery Cold Drawing BHN
≤262
condition of delivery Annealing BHN
≤235
specimen Preheat at 788±14 ℃, heat at 1204±5.6℃(controllable atmosphere) or 1191℃(salt bath), hold for 5 to 15 min,air cool. Temper twice at 552±5.6℃, each time for 2 h HRC
≥60
A681TypeH42 Corresponding Standards(Same grade name, different standards)