Grade A681 Type S4
USA UNS T41904
AISI
American Iron and Steel Institute
S4
Corresponding Standard ASTM A681-2024
Tool Steels Alloy
Classification Tool Steel
A681 Type S4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr V More
Minimum Value 0.5 1.75 0.6 - - 0.1 0.15 Ni+Cu≤0.75
Maximum Value 0.65 2.25 0.95 0.03 0.03 0.5 0.35
A681 Type S4 Mechanical Properties
condition Heat Treatment or Condition
Hardness
HBW
condition of delivery Cold Drawing BHN
≤255
condition of delivery Annealing BHN
≤229
specimen Preheat at 677±14 ℃, heat at 899±5.6℃(controllable atmosphere) or 885℃(salt bath), hold for 5 to 15 min, oil cool. Temper at 204±5.6℃ once for 2 h HRC
≥58
A681TypeS4 Corresponding Standards(Same grade name, different standards)

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!