Grade GX4CrNi13-4
European Standard Steel Grade 1.4317
Corresponding Standard EN 10283-2019
Corrosion Resistant Steel Castings
Classification Cast Steel
Density 7.7 g/cm3
GX4CrNi13-4 Chemical Element Composition Content (%)
Component C Si Mn P S Cr Ni Cu Mo V
Minimum Value - - - - - 12 3.5 - - -
Maximum Value 0.06 1 1 0.035 0.025 13.5 5 0.3 0.7 0.08
GX4CrNi13-4 Mechanical Properties
thickness
t
mm
Heat Treatment or Condition
Tensile Strength
σb
Mpa
Specified Plastic Yield Strength
Rp0.2
Mpa
Elongation or Extension Rate
δ
%
Impact Energy Absorption
KV2
J
t≤300 Quench in air or liquid at 1000~1050°C and temper at 590-620°C (+QT) ≥760 ≥550 ≥15 ≥50
t≤300 Quench in air or liquid at 1000~1050°C and temper at 500-530°C (+QT) ≥900 ≥830 ≥12 ≥35
t≤300 1000-1050°C air or liquid quenching + first tempering 660-680°C, second tempering 560-620°C (+QT) ≥700 ≥500 ≥16 ≥50

Note: The data is for reference only! If you have any questions, please fill out "I want to correct it"!